Active standard ASTM F88/F88M-23, the Standard Test Method for Seal Strength of Flexible Barrier Materials, measures the force required to separate a test strip of material containing a seal and identifies the mode of specimen failure (Clauses 1.1 and 1.4). Because part of the measured separation force may be a bending component rather than seal strength alone, Clause 4.2 recommends consistent use of a single tail-holding geometry—Technique A (unsupported), Technique B (hand-supported at 90° to the tails), or Technique C (supported 180° against a rigid alignment plate or package structure)—throughout an entire test series.

Clause 4.1.1 states that maximum seal force is important information, and for applications where average force to separate the seal is useful, average force should also be reported. Note 1 cautions that strip separation reflects the sampled area of the package and does not simulate a user interfacing with an entire package during opening. Within packaging safety records, a strip peel force is not a whole-package leak result: establish the seal object, sample, observation, and reject path through seal integrity questions, and select whole-package bubble, vacuum-decay, or nonporous dye checks on seal integrity testing with ASTM methods.

What Seal Properties Does ASTM F88 Measure on Flexible Barrier Strips?

ASTM F88/F88M-23 covers the measurement of seal strength in flexible barrier materials (Clause 1.1), whether the seal joins a flexible material to another flexible material, a rigid material, or a semi-rigid material (Clause 1.2). On each cut strip, the seal peel test records two linked outputs: the force required to separate the strip across the seal and the mode of specimen failure (Clause 1.4). Clause 1.5 distinguishes this strip method from Test Method F2824, which measures mechanical seal strength while separating an entire lid (cover or membrane) from a rigid or semi-rigid round container.

Clause 4.1 defines seal strength as a quantitative measure for process validation, capability, and control. The measurement relates to opening force, package integrity, and the packaging process ability to produce consistent seals (Clause 4.1). Note 1 adds that seal-strength values measure the output of seal separation and may also involve mechanical properties of the materials forming the seal, because those substrates can deform or elongate during the test.

Lower and upper seal-strength specifications serve distinct packaging functions under Clause 4.1 and Notes 2 and 3:

  • Minimum closure assurance (Clause 4.1 and Note 2): Seal strength at some minimum level is a necessary package requirement, and lower seal-strength specifications are typically utilized to provide assurance of package closure, which can contribute to seal integrity.
  • Peelable seal opening limits (Clause 4.1 and Note 3): At times an upper limit to seal strength is desirable to facilitate opening; upper seal-strength specifications are typically utilized to limit the force required so an end user is able to open the design, and are typically limited to peelable seals intended to be peeled by the end user.

How Does Technique A Differ From Supported Tail-Holding Fixtures?

On a peel strength tester equipped with opposing grips, tail angle changes how much bending resistance enters the force reading. Clause 4.2 states that a portion of the force measured when testing materials may be a bending component and not seal strength alone. Fixtures and holding techniques position samples at controlled angles to the pull direction to manage that bending component, as illustrated in Fig. 1 of the standard (Clause 4.2). Because each holding approach affects test results differently, Clause 4.2 recommends consistent use of one technique—Technique A, Technique B, or Technique C—throughout a test series.

Three-panel geometry schematic of ASTM F88/F88M-23 Technique A unsupported, Technique B hand-supported at 90 degrees with loose contact, and Technique C folded 180 degrees against a rigid alignment plate.
ASTM F88/F88M-23 Clauses 4.2.1 to 4.2.3 define three tail-holding geometries that change the bending component; one technique stays fixed across a test series.
Holding Technique ASTM F88/F88M-23 Clause Grip and Tail Geometry Operational Controls and Fixtures
Technique A: Unsupported Clause 4.2.1 Each specimen tail is secured in opposing grips while the seal remains unsupported during the pull Flexible tails can move or flip during testing, which may impact measured strength and should be reported with results (Note 5)
Technique B: Supported 90° (By Hand) Clause 4.2.2 and Note 4 Each specimen tail is secured in opposing grips while the seal stays hand-supported at a 90° perpendicular angle to the tails Hand contact is intended to be loose, only preventing tail movement up or down; actual gripping or excessive lateral hand force impacts results
Technique C: Supported 180° Clause 4.2.3 For flexible-to-flexible seals, the least flexible tail is typically supported flat against a rigid alignment plate in one grip and the more flexible tail is typically folded 180° over the seal in the opposing grip In rigid and semi-rigid applications, the package structure may be maintained on the least flexible side and gripped or fixtured

Note 6 emphasizes that test method validation should account for fixtures or alignment plates as well as which material is placed into which grip, since both factors are known to impact results and depend on package design features. Note 6 points to Guide F3263 for guidance on test method validation and notes that Appendix X4 includes examples of optional fixtures and equipment with built-in fixturing.

What Does the ASTM F88/F88M Designation Cover Across Seal Materials?

The active ASTM store listing designates the standard as ASTM F88/F88M-23 in Book of Standards Volume 15.10, developed by Subcommittee F02.20, spanning 20 pages under DOI 10.1520/F0088_F0088M-23 and ICS code 55.040. Clause 1.3 states that seals tested under this method may come from any source, laboratory or commercial. Clause 1.7 places responsibility on the user of the standard to establish appropriate safety, health, and environmental practices and to determine the applicability of regulatory limitations prior to use.

The dual F88/F88M designation reflects two separate unit systems governed by Clause 1.6. Values stated in either SI units or inch-pound units are regarded separately as standard. Because values in each system may not be exact equivalents, each system shall be used independently of the other, and combining values from the two systems may result in non-conformance with the standard (Clause 1.6).

Published research illustrates why laboratory test records have to document exact protocol settings alongside the standard designation. A packaging-materials review citing ASTM F88/F88M-23 notes that seal-strength values in the literature come from protocols—including ASTM F88 and DIN 55529—that differ in peel angle, seal bar geometry, specimen conditioning, and loading rate, creating heterogeneity that limits cross-study comparability:

  • A flexible-food-packaging study reports seal strength in gf under ASTM F88/F88M-23 and lists lamination strength in gf on a separate row under ASTM F88/F88M-23.
  • A flexible-film study following ASTM F88/F88M-21 specifies its own setup: a 500 N load cell, a 25 mm jaw separation, a 250 mm/min crosshead speed, and the non-supported seal technique.
  • Another film study measuring seal strength under ASTM F88/F88M-23 prepared 10 by 2.5 cm film strips conditioned at 53% RH for one week prior to testing.
  • A coating T-peel study conforming to the earlier ASTM F88-07a edition ran its evaluation at a 300 mm/min crosshead speed.

Each of those loading rates, jaw gaps, strip dimensions, and conditioning steps belongs to the individual study’s documented procedure.

How Does Peel Strength Testing Differ From ASTM F1929 Dye Leak Checks?

ASTM F88/F88M-23 measures mechanical separation force and specimen failure mode on a cut seal strip (Clause 1.4), whereas ASTM F1929-23, Standard Test Method for Detecting Seal Leaks in Porous Medical Packaging by Dye Penetration, visually locates channel defects in porous medical package edge seals. F1929-23 Clause 4.1 notes that harmful biological or particulate contaminants may enter a medical package through leaks frequently found at seals between same or dissimilar components, or through pinholes in packaging material.

F1929-23 applies strictly to transparent-to-porous edge seals rather than nonporous food pouches:

  • Channel threshold and materials (Clauses 1.1, 1.3, and 1.4): F1929-23 defines procedures to detect and locate a leak equal to or greater than a channel formed by a 50 µm (0.002 in.) wire in package edge seals formed between a transparent material and a porous sheet material, using a dye penetrant solution with good contrast to the opaque packaging material.
  • Application methods and visual inspection (Clauses 1.1, 1.2, and 4.2): Dye penetrant is applied locally via injection, edge dip, or eyedropper; after contact for a specified time, the seal edge is visually inspected to observe channel defects by dye leakage.
  • Qualitative pass/fail scope (Clauses 4.3, 4.4, and 4.5): The procedure applies only to individual seal leaks rather than multiple small leaks in porous packaging material. It is not quantitative, gives no indication of leak size, and is usually employed as a pass/fail test in which components showing any leakage indication are normally rejected.
  • Wicking and paper limits (Clauses 1.3 and 4.6): The porous sheet material has to retain the dye solution and keep it from discoloring the seal area for a minimum of 5 seconds; dye wicks through porous material over time (verifiable on the porous side of the seal), and uncoated papers are especially susceptible to leakage and must be evaluated carefully for use with each method.

For nonporous flexible food seals, compare the nonporous dye, vacuum-decay, and bubble-emission leak methods on seal integrity testing with ASTM methods rather than assigning F1929-23.

When Should Seal Peel Checks Be Paired With ASTM F2096 Bubble Tests?

Pair strip peel testing with whole-package leak testing when a packaging qualification or line audit asks both how much force separates a sampled seal strip and whether whole packages exhibit gross leaks. Lower seal-strength specifications under ASTM F88/F88M-23 Note 2 can contribute to seal integrity by supporting package closure assurance, yet strip separation force only characterizes the sampled strip area (Note 1). Consistent with that boundary, the flexible-food-packaging study records seal strength under ASTM F88/F88M-23 and vacuum tightness under ASTM D3078-02 as separate rows, and our neighbor guide on seal integrity testing with ASTM methods notes that no peel-strength requirement is inferred from leak methods.

When gross-leak testing uses internal air pressure, ASTM F2096-11(2019), Standard Test Method for Detecting Gross Leaks in Packaging by Internal Pressurization (Bubble Test), provides a practical way to examine tray and pouch packages—including large or long packages that do not fit other integrity apparatus—for gross leaks, substrate holes, and channels (Clauses 1.1, 5.1, 5.3, 5.4, and 5.5). Clause 5.4 notes that package integrity is crucial to consumer safety because heat-sealed packages are designed to provide a contamination-free or sterile environment, or both, to the product. Three F2096-11(2019) scope boundaries govern how its record is written:

  1. Evaluated sensitivity scope (Clauses 1.1 and 1.2): Clause 1.1 states method sensitivity down to 250 μm (0.010 in.) with an 81% probability, while Clause 1.2 specifies that sensitivity has not been evaluated for porous materials other than spunbonded polyolefin or for nonporous packaging.
  2. Destructive package entry (Clause 1.3): F2096-11(2019) is destructive because it requires entry into the package to supply internal air pressure.
  3. Standard units (Clause 1.4): Values stated in SI units are regarded as the standard, and parenthetical values are for information only.

In regulated sterile medical and pharmaceutical stability programs—distinct from food-pouch rules—the February 2008 FDA guidance on container and closure system integrity testing addresses sterile biological products, human and animal drugs, and medical devices. That guidance lists bubble tests, pressure/vacuum decay, trace gas permeation/leak tests, dye penetration tests, and seal force among example physical integrity methods, states that FDA guidance documents do not establish legally enforceable responsibilities unless specific regulatory or statutory requirements are cited, explains that an integrity method is adequately validated when proven through scientifically accepted studies to detect a breach, and specifies that integrity tests do not replace sterility testing prior to product release.

How Are Maximum Force, Average Force, and Failure Modes Recorded?

Under ASTM F88/F88M-23 Clauses 1.4 and 4.1.1, each test series records the maximum seal force, the average force to separate the seal when useful for the application, and the mode of specimen failure. Note 5 adds that any tail movement or flipping during the pull should be reported with results, and Note 6 states that test method validation should account for use of fixtures or alignment plates and which material is placed into which grip.

Published film studies citing ASTM F88/F88M-21 illustrate how researchers describe specimen failure modes in words alongside force data:

  • One flexible-film study reported that its films exhibited adhesive failures under all tested conditions according to ASTM F88/F88M-21, except under certain conditions where a material break occurred.
  • Another film study citing Method F88/F88M-21 (DOI 10.1520/F0088_F0088M-21) reported that all specimens exhibited ductile failure—elongation followed by rupture within or near the sealed region—indicating cohesive rather than adhesive failure.
Structured seal-testing record form with fields for single tail-holding technique, unit system, maximum force, optional average force, failure mode, tail-flip note, and a separate package leak-method row.
Bench record layout keeping single-technique peel forces, specimen failure modes, and tail-flip notes separate from any whole-package leak test.

Use one row per test series to keep the strip peel record and any companion leak test distinct:

Series Record Field What to Record Method Boundary
Tail-holding technique Single geometry used across the entire series: Technique A (unsupported), Technique B (supported 90° by hand, loose contact), or Technique C (supported 180°) Mixing holding techniques within a series alters the bending component of measured force (Clause 4.2 and Note 4)
Grip assignment and fixture Which substrate is clamped in each grip, plus rigid alignment plate or package-structure fixture details Grip orientation and fixturing impact measured seal strength and belong in method validation (Clause 4.2.3 and Note 6)
Maximum seal force and unit system Peak separation force in either SI units or inch-pound units used independently SI and inch-pound values may not be exact equivalents and are not combined (Clauses 1.6 and 4.1.1)
Average seal force (when used) Average separation force when required by the application, or a dash (—) when only maximum force is tracked Reported alongside maximum seal force for applications where average separation force is useful (Clause 4.1.1)
Specimen failure mode and tail flip Observed failure mode on the strip (such as adhesive failure, cohesive ductile rupture, or material break) plus any tail movement or flipping Clause 1.4 pairs force with failure mode; Note 5 flags tail flipping because it can impact measured strength
Separate leak-check method (if run) Exact whole-package leak standard and edition, tested lot, observed indication, and hold owner linked to seal integrity questions Strip peel strength does not establish whole-package leak absence; record leak checks on a separate line